骨瓷釉系列介绍
Bone china glaze series introduction
品名 |
编号 |
烧成温度 |
体膨胀 |
使用说明 |
Type |
Item No |
Tempreture |
COE |
Application |
新瓷器 fine china |
DP-1 |
1120-1140℃ |
152 |
The operation steps as follows
1.Add more than 30% water into the glaze lump, mix completely and leave for over 2hours.
2.Loading the glaze into mill machine grind 2 hours.
3.removing iron and filtration , sieving through 200 mesh.
4.adjust density to 60-65 degree.
5. keep the high gap at the 1-1.5 meters from the glaze tub to spray gun.
6.install a pressure regulator in front of spray gun, and adjust the pressure at the 0.8-1.2mm.
7.after glaze firing temperature reach to setting degree. Keep heat on 20-25 minutes.
8.after heat preservation open the kiln door by a third.
9.quickly cool itself. The glaze will achieve to good effect.
操作步骤如下:
1.将30%以上的水加入釉块内,平均浸泡2小时以上
2.将釉料装入球磨机内磨2小时.
3.除铁和过滤,通过200目筛。
4.调整浓度为60-65度.
5.釉桶与喷枪高位差距为1-1.5米。
6.在喷枪前安装压力调节器,调节压力为2Mpa,喷釉厚度为0.8-1.2mm.
7.釉烧后温度达到设定度,保温20-25分钟。
8.保温后,将窑门打开三分之一。
9.即速自然降温,釉面达到更佳效果
|
新骨瓷 New bone |
BO-3 |
1120-1140℃ |
208 |
老瓷器 old china |
DP-1 |
1120-1140℃ |
152 |
BO-3 |
1120-1140℃ |
208 |